With excellent mechanical and processing properties, it is widely used in automobiles, household appliances, mechanical parts and so on. Its manufacturing process is mainly cold rolling, which can make the surface of steel more smooth, and improve the surface quality including dimensional accuracy of steel.
| Grade | C | Si | Mn | P | S | AI | Cu | Ti+Nb | Cr+Mo | B |
| Max % | Max % | Max % | Max % | Max % | Range % | Max % | Max % | Max % | Max % | |
| DPC290Y490T | 0.14 | 0.50 | 1.8 | 0.080 | 0.015 | 0.01-1.0 | 0.20 | 0.15 | 1.00 | 0.005 |
| DPC340Y590T | 0.15 | 0.75 | 2.5 | 0.080 | 0.015 | 0.01-1.5 | 0.20 | 0.15 | 1.40 | 0.005 |
| DPC420Y780T | 0.18 | 0.80 | 2.5 | 0.080 | 0.015 | 0.01-2.0 | 0.20 | 0.15 | 1.40 | 0.005 |
| DPC420Y780T HF | 0.18 | 1.00 | 2.5 | 0.080 | 0.015 | 0.01-2.0 | 0.20 | 0.15 | 1.40 | 0.005 |
| DPC550Y980T | 0.20 | 1.00 | 2.9 | 0.080 | 0.015 | 0.01-2.0 | 0.20 | 0.15 | 1.40 | 0.005 |
| DPC700Y980T | 0.23 | 1.00 | 2.9 | 0.080 | 0.015 | 0.01-2.0 | 0.20 | 0.15 | 1.40 | 0.005 |
| DPC950Y1180T | 0.23 | 0.40 | 2.9 | 0.080 | 0.015 | 0.01-2.0 | – | 0.15 | 1.40 | 0.005 |
| DPH330Y580T | 0.14 | 1.00 | 2.2 | 0.085 | 0.015 | 0.015-1.0 | 0.40 | 0.15 | 1.40 | 0.005 |
NOTE 1: In addition to requirements shown in the table, %Ni+%Cr+%Mo < 1.5.
NOTE 2: All DP grades with C% <0.015 must have a minimum of 0.0003% (3 ppm) Boron.
NOTE 4: Ceq. max. 0.86 – Ceq. = C+(Mn+Si)/6.
NOTE 5: Si + Al max. 2.0.
| Dual Phase CR Grade | YS Range (MPa) | TS (MPa) min | A50 % min | A80 % min | n4-6% min | n10%-UE min | BH2 min |
| DPC290Y490T | 290-380 | 490 | 26 | 24 | 0.19 | 0.15 | 30 |
| DPC340Y590T | 340-440 | 590 | 21 | 20 | 0.18 | 0.14 | 30 |
| DPC420Y780T | 420-550 | 780 | 15 | 14 |
0.15
0.12(1) |
0.11 | 30 |
| DPC420Y780T HF(2) | 420-560 | 780 | 18 | 17 | 0.17 | 0.14 | 30 |
| DPC550Y980T | 550-730 | 980 | 9 | 8 | 0.08 | N/A | 30 |
| DPC700Y980T | 700-850 | 980 | 8 | 7 | N/A | N/A | 30 |
| DPC950Y1180T | 830-1130 | 1180 | 5 | 4 | N/A | N/A | 30 |
NOTE 1: Valid only for NA production.
NOTE 2: High Formability quality of DP780 grade.
| Dual Phase CR Grade | YS Range (MPa) | TS (MPa) min | A50 % min | A80 % min | n4-6% min | n10%-UE min | BH2 min |
| DPH330Y580T | 330-450 | 580 | 21 | 19 | 0.16 | 0.13 | 30 |