Galvanized steel plate is immersed in molten zinc liquid to form zinc layer protection and improve corrosion resistance and durability. Commonly used in construction, automotive and other fields.
| Composition, %—Heat Analysis Element, max (unless otherwise shown) | ||||||||||||
| Designation | Carbon | Manganese | Phosphorus | Sulfur | Aluminum min | Cu | Ni | Cr | Mo | V | Cb | TiB |
| CS TypeA C,D,E | 0.1 | 0.6 | 0.03 | 0.035 | – | 0.25 | 0.2 | 0.15 | 0.06 | 0.008 | 0.008 | 0.025 |
| CS TypeB F,C | 0.02 to 0.15 | 0.6 | 0.03 | 0.035 | – | 0.25 | 0.2 | 0.15 | 0.06 | 0.008 | 0.008 | 0.025 |
| CS TypeC C,D,E | 0.08 | 0.6 | 0.1 | 0.035 | – | 0.25 | 0.2 | 0.15 | 0.06 | 0.008 | 0.008 | 0.025 |
| FS TypeA C,G | 0.1 | 0.5 | 0.02 | 0.035 | – | 0.25 | 0.2 | 0.15 | 0.06 | 0.008 | 0.008 | 0.025 |
| FS TypeB F,C | 0.02 to 0.10 | 0.5 | 0.02 | 0.035 | – | 0.25 | 0.2 | 0.15 | 0.06 | 0.008 | 0.008 | 0.025 |
| DDS TypeA D,E | 0.06 | 0.5 | 0.02 | 0.025 | 0.01 | 0.25 | 0.2 | 0.15 | 0.06 | 0.008 | 0.008 | 0.025 |
| DDS TypeC H | 0.02 | 0.5 | 0.020 to 0.100 | 0.025 | 0.01 | 0.25 | 0.2 | 0.15 | 0.06 | 0.1 | 0.1 | 0.15 |
| EDDSH | 0.02 | 0.4 | 0.020 to 0.100 | 0.02 | 0.01 | 0.25 | 0.2 | 0.15 | 0.06 | 0.1 | 0.1 | 0.15 |
A Where an ellipsis (. . .) appears in this table, there is no requirement, but the analysis shall be reported.
B For steels containing more than 0.02 % carbon, titanium is permitted at the producer’s option, to the lesser of 3.4N + 1.5S or 0.025 % for the purpose of stabilization.
C When a deoxidized steel is required for the application, the purchaser has the option to order CS and FS to a minimum of 0.01 % total aluminum.
D Steel is permitted to be furnished as a vacuum degassed or chemically stabilized steel, or both, at the producer’s option.
E For carbon levels less than or equal to 0.02 %, vanadium, columbium, or titanium, or combinations thereof are permitted to be used as stabilizing elements at the producer’s option. In such cases, the applicable limit for vanadium and columbium shall be 0.10 % max and the limit for titanium shall be 0.15 % max.
F For CS and FS, specify Type B to avoid carbon levels below 0.02 %.
G Shall not be furnished as a stabilized steel.
H Shall be furnished as a stabilized steel.
| Composition, %—Heat Analysis Element, max (unless otherwise shown) | |||||||||||
| Designation | Carbon | Manganese | Phosphorus | Sulfur | Cu | Ni | Cr | Mo | VB | CbB | TiB,C,D |
| SS | 0.2 | 1.35 | 0.04 | 0.04 | 0.25 | 0.2 | 0.15 | 0.06 | 0.008 | 0.008 | 0.025 |
| 33 [230] | 0.2 | 1.35 | 0.1 | 0.04 | 0.25 | 0.2 | 0.15 | 0.06 | 0.008 | 0.008 | 0.025 |
| 37 [255] | 0.25 | 1.35 | 0.1 | 0.04 | 0.25 | 0.2 | 0.15 | 0.06 | 0.008 | 0.008 | 0.025 |
| 40 [275] | 0.25 | 1.35 | 0.2 | 0.04 | 0.25 | 0.2 | 0.15 | 0.06 | 0.008 | 0.008 | 0.025 |
| 50 [340] Class 1, 2, and 4 | 0.25 | 1.35 | 0.04 | 0.04 | 0.25 | 0.2 | 0.15 | 0.06 | 0.008 | 0.008 | 0.025 |
| 55 [380] | 0.25 | 1.35 | 0.04 | 0.04 | 0.25 | 0.2 | 0.15 | 0.06 | 0.008 | 0.008 | 0.025 |
| 80 [550] Class 1 | 0.2 | 1.35 | 0.04 | 0.04 | 0.25 | 0.2 | 0.15 | 0.06 | 0.008 | 0.015 | 0.025 |
| 80 [550] Class 2E | 0.02 | 1.35 | 0.05 | 0.02 | 0.25 | 0.2 | 0.15 | 0.06 | 0.1 | 0.1 | 0.15 |
| HSLASF 40 [275] | 0.2 | 1.2 | – | 0.035 | – | 0.2 | 0.15 | 0.16 | 0.01 min | 0.005 min | 0.01 min |
| 50 [340] | 0.2 | 1.2 | – | 0.035 | 0.2 | 0.2 | 0.15 | 0.16 | 0.01 min | 0.005 min | 0.01 min |
| 55 [380] Class 1 | 0.25 | 1.35 | – | 0.035 | 0.2 | 0.2 | 0.15 | 0.16 | 0.01 min | 0.005 min | 0.01 min |
| 55 [380] Class 2 | 0.15 | 1.2 | – | 0.035 | 0.2 | 0.2 | 0.15 | 0.16 | 0.01 min | 0.005 min | 0.01 min |
| 60 [410] | 0.2 | 1.35 | – | 0.035 | 0.2 | 0.2 | 0.15 | 0.16 | 0.01 min | 0.005 min | 0.01 min |
| 70 [480] | 0.2 | 1.65 | – | 0.035 | 0.2 | 0.2 | 0.15 | 0.16 | 0.01 min | 0.005 min | 0.01 min |
| 80 [550] | 0.2 | 1.65 | – | 0.035 | 0.2 | 0.2 | 0.15 | 0.16 | 0.01 min | 0.005 min | 0.01 min |
| HSLAS-FF,G 40 [275] | 0.15 | 1.2 | – | 0.035 | – | 0.2 | 0.15 | 0.16 | 0.01 min | 0.005 min | 0.01 min |
| 50 [340] | 0.15 | 1.2 | – | 0.035 | 0.2 | 0.2 | 0.15 | 0.16 | 0.01 min | 0.005 min | 0.01 min |
| 55 [380] Class 1 | 0.2 | 1.35 | – | 0.035 | 0.2 | 0.2 | 0.15 | 0.16 | 0.01 min | 0.005 min | 0.01 min |
| 55 [380] Class 2 | 0.15 | 1.2 | – | 0.035 | 0.2 | 0.2 | 0.15 | 0.16 | 0.01 min | 0.005 min | 0.01 min |
| 60 [410] | 0.15 | 1.2 | – | 0.035 | 0.2 | 0.2 | 0.15 | 0.16 | 0.01 min | 0.005 min | 0.01 min |
| 70 [480] | 0.15 | 1.65 | – | 0.035 | 0.2 | 0.2 | 0.15 | 0.16 | 0.01 min | 0.005 min | 0.01 min |
| 80 [550] | 0.15 | 1.65 | – | 0.035 | 0.2 | 0.2 | 0.15 | 0.16 | 0.01 min | 0.005 min | 0.01 min |
| SHSD | 0.12 | 1.5 | 0.12 | 0.03 | 0.2 | 0.2 | 0.15 | 0.16 | 0.008 | 0.008 | 0.025 |
| BHSD | 0.12 | 1.5 | 0.12 | 0.03 | 0.2 | 0.2 | 0.15 | 0.16 | 0.008 | 0.008 | 0.025 |
A Where an ellipsis (. . .) appears in this table there is no requirement, but the analysis shall be reported.
B For carbon levels less than or equal to 0.02 %, vanadium, columbium, or titanium, or combinations thereof, are permitted to be used as stabilizing elements at the producer’s option. In such cases, the applicable limit for vanadium and columbium shall be 0.10% max., and the limit for titanium shall be 0.15 % max.
C Titanium is permitted for SS steels at the producer’s option, to the lesser of 3.4N +1.5S or 0.025 % for the purpose of stabilization.
D For steels containing more than 0.02 % carbon, titanium is permitted to the lesser of 3.4N + 1.5S or 0.025 %.
E Shall be furnished as a stabilized steel.
F HSLAS and HSLAS-F steels commonly contain the strengthening elements columbium, vanadium, and titanium added singly or in combination. The minimum requirements only apply to the microalloy elements selected for strengthening of the steel.
G HSLAS-F steel shall be treated to achieve inclusion control.
| Designation | Grade | Yield Strength min, ksi | Tensile Strength min, ksiA | Elongation in 2 in min, %A | Bake Hardening Index, min, ksi Upper Yield/Lower YieldA |
| SS | 33 | 33 | 45 | 20 | – |
| 37 | 37 | 52 | 18 | – | |
| 40 | 40 | 55 | 16 | – | |
| 50 Class 1 | 50 | 65 | 12 | – | |
| 50 Class 2 | 50 | – | 12 | – | |
| 50 Class 3 | 50 | 70 | 12 | – | |
| 50 Class 4 | 50 | 60 | 12 | – | |
| 55 | 55 | 70 | 11 | – | |
| 80 Class 1B | 80C | 82 | – | – | |
| 80 Class 2B,D | 80C | 82 | – | – | |
| HSLAS | 40 | 40 | 50E | 22 | – |
| 50 | 50 | 60E | 20 | – | |
| 55 Class 1 | 55 | 70E | 16 | – | |
| 55 Class 2 | 55 | 65E | 18 | – | |
| 60 | 60 | 70E | 16 | – | |
| 70 | 70 | 80E | 12 | – | |
| 80 | 80 | 90E | 10 | – | |
| HSLAS-F | 40 | 40 | 50E | 24 | – |
| 50 | 50 | 60E | 22 | – | |
| 55 Class 1 | 55 | 70E | 18 | – | |
| 55 Class 2 | 55 | 65E | 20 | – | |
| 60 | 60 | 70E | 18 | – | |
| 70 | 70 | 80E | 14 | – | |
| 80 | 80 | 90E | 12 | – | |
| SHSD | 26 | 26 | 43 | 32 | – |
| 31 | 31 | 36 | 30 | – | |
| 35 | 35 | 50 | 26 | – | |
| 41 | 41 | 53 | 24 | – | |
| 44 | 44 | 57 | 22 | – | |
| BHS | 26 | 26 | 43 | 30 | 4/3 |
| 31 | 31 | 46 | 28 | 4/3 | |
| 35 | 35 | 50 | 24 | 4/3 | |
| 41 | 41 | 53 | 22 | 4/3 | |
| 44 | 44 | 57 | 20 | 4/3 |
| Designation | Grade | Yield Strength min, ksi | Tensile Strength min, ksiA | Elongation in 2 in min, %A | Bake Hardening Index, min, ksi Upper Yield/Lower YieldA |
| SS | 230 | 230 | 310 | 20 | – |
| 255 | 255 | 360 | 18 | – | |
| 275 | 275 | 380 | 16 | – | |
| 340 Class 1 | 340 | 450 | 12 | – | |
| 340 Class 2 | 340 | – | 12 | – | |
| 340 Class 3 | 340 | 480 | 12 | – | |
| 340 Class 4 | 340 | 410 | 12 | – | |
| 380 | 380 | 480 | 11 | – | |
| 550 Class 1B | 550c | 570 | – | – | |
| 550 Class 2B,D | 550c | 570 | – | – | |
| HSLAS | 275 | 275 | 340E | 22 | – |
| 340 | 340 | 410E | 20 | – | |
| 380 Class 1 | 380 | 480E | 16 | – | |
| 380 Class 2 | 380 | 450E | 18 | – | |
| 410 | 410 | 480E | 16 | – | |
| 480 | 480 | 450E | 12 | – | |
| 550 | 550 | 480E | 10 | – | |
| HSLAS-F | 275 | 275 | 550E | 24 | – |
| 340 | 340 | 620E | 22 | – | |
| 380 Class 1 | 380 | 480E | 18 | – | |
| 380 Class 2 | 380 | 450E | 20 | – | |
| 410 | 410 | 480E | 18 | – | |
| 480 | 480 | 550E | 14 | – | |
| 550 | 550 | 620E | 12 | – | |
| SHSD | 180 | 180 | 300 | 32 | – |
| 210 | 210 | 320 | 30 | – | |
| 240 | 240 | 340 | 26 | – | |
| 280 | 280 | 370 | 24 | – | |
| 300 | 300 | 390 | 22 | – | |
| BHS | 180 | 180 | 300 | 30 | 25/20 |
| 210 | 210 | 320 | 28 | 25/20 | |
| 240 | 240 | 340 | 24 | 25/20 | |
| 280 | 280 | 370 | 22 | 25/20 | |
| 300 | 300 | 390 | 20 | 25/20 |
| Designation | Yield Strength | Elongation in 2 in. [50 mm], % | rm Value C | n ValueD | |
| ksi | [MPa] | ||||
| CS Type A | 25/55 | [170/380] | ≥20 | E | E |
| CS Type B | 30/55 | [205/380] | ≥20 | E | E |
| CS Type C | 25/60 | [170/410] | ≥15 | E | E |
| FS Types A and B | 25/45 | [170/310] | ≥26 | 1.0/1.4 | 0.17/0.21 |
| DDS Type A | 20/35 | [140/240] | ≥32 | 1.4/1.8 | 0.19/0.24 |
| DDS Type C | 25/40 | [170/280] | ≥40 | 1.2/1.8 | 0.17/0.24 |
| EDDSF | 15/25 | [105/170] | ≥40 | 1.6/2.1 | 0.22/0.27 |
A The typical mechanical property values presented here are nonmandatory. They are intended solely to provide the purchaser with as much information as possible to make an informed decision on the steel to be specified. Values outside of these ranges are to be expected. The purchaser may negotiate with the supplier if a specific range or a more restrictive range is required for the application.
B These typical mechanical properties apply to the full range of steel sheet thicknesses. The yield strength tends to increase and some of the formability values tend to decrease as the sheet thickness decreases.
C rm Value—Average plastic strain ratio as determined by Test Method E 517.
D n Value—Strain-hardening exponent as determined by Test Method E 646.
E No typical mechanical properties have been established.
F EDDS Sheet will be free from changes in mechanical properties over time, that is, nonaging.